高级检索

    TA31合金冷轧管件断后伸长率偏低原因

    Reasons for the low elongation after fracture of TA31 alloy cold-rolled pipe fittings

    • 摘要: 某石化装备用TA31合金冷轧管件出现断后伸长率异常偏低的现象。采用宏观观察、化学成分分析、力学性能测试、扫描电镜及能谱分析、金相检验等方法对管件断后伸长率偏低的原因进行分析。结果表明:管件内表面存在α层和折叠缺陷,使试样表面在拉伸试验过程中产生应力集中并萌生裂纹,改变了试样的受力状态,最终导致管件的断后伸长率降低。

       

      Abstract: The TA31 alloy cold-rolled pipe fittings used in a certain petrochemical equipment exhibit abnormally low elongation after fracture. The reasons for the low elongation after fracture of the pipe fittings were analyzed using macroscopic observation, chemical composition analysis, mechanical property testing, scanning electron microscopy and energy spectrum analysis, metallographic examination. The results show that there were α layers and folding defects on the inner surface of the pipe fittings, which led to stress concentration and crack initiation on the surface of the specimen during the tensile test, changed the stress state of the specimen and ultimately resulted in a decrease in the elongation after fracture of the pipe fittings.

       

    /